Silicone rubber transfer printing process with forward rotation


Operation process of forward transfer:

  1. Apply hot melt adhesive W-9710-6 six times, with surface drying after each application.
  2. Print twice with W-9714-1 special silicone rubber and 10% G-014 additive. The first print dries on the surface, and the second print does not require baking.
  3. Print 5-8 times with W-9802 right-angle silicone and 10% G085 additive, with surface treatment each time.
  4. Apply W-9802 right-angle silicone rubber, 10% color paste, and 10% G085, printing 3 times, with each application being surface treatment.
  5. Print once with W-9705-3 matte silicone + 4% G-010 additive, and allow surface drying.
    Note: After printing, place in a sealed oven and bake at 100℃ for 2 hours. Press machine: 150℃ for 15 seconds with a pressure of 4kg